做了个涂层热应力分析,大家指点一下!
我是初学者!在WC上有涂层TiC,从加工温度600度,降到室温20时产生热应力,程序如下,建了个二维模型,不知道这个模型可用不,请大家指教!fini
/clear
!define martiral parameters
!1-WC,2-TiC
tec1=4.5e-6 !thermal expansion officient ℃^ -1
tec2=7.1e-6
e1=4.1e11 !Yang's modulus(pa)
e2=3.4e11
p1=0.28 !Poisson ratio
p2=0.19
TEMPref=600 !℃
TEMPnow=20
!define geometrical parameters
x=1e-4 ! width
y1=2e-5 ! thickness of the substrate
y2=2e-6 ! thickness of the coating
/prep7
rect,,x,,y1
rect,,x,y1,y1+y2
aglue,all
!define martial porperties
et,1,13,4,,1
!martiral poperties
MP,EX,1,e1
MP,PRXY,1,p1
MP,ALPX,1,tec1
MP,EX,2,e2
MP,PRXY,2,p2
MP,ALPX,2,tec2
!mesh area
!mesh the substrate
lsel,s,loc,y,0
LESIZE,all,,,20,0.2,
lsel,all
lsel,s,loc,y,y1
lsel,a,loc,y,y1+y2
LESIZE,all,,,20,5,
lsel,all
asel,s,loc,y,1e-5
lsla
lsel,r,loc,x,0
LESIZE,all,,,10,5,,
allsel
asel,s,loc,y,1e-5
lsla
lsel,r,loc,x,x
LESIZE,all,,,10,0.2,,
allsel
asel,s,loc,y,1e-5
type,1
mat,1
mshape,0,2D
mshkey,1
amesh,all
allsel
!mesh the coating
asel,s,loc,y,2.1e-5
lsla
lsel,r,loc,x,0
LESIZE,all,0, ,6,5,4,0,0
allsel
asel,s,loc,y,2.1e-5
lsla
lsel,r,loc,x,x
lesize,all,,,6,5
allsel
asel,s,loc,y,2.1e-5
type,1
mat,2
mshape,0,2D
mshkey,1
amesh,all
allsel
/solu
tunif,TEMPnow
tref,TEMPref
NSEL,s,LOC,X,0
D,ALL,UX
ALLSEL,ALL
NSEL,s,LOC,y,0
D,ALL,Uy
ALLSEL,ALL
solve 下面是这个程序得到的结果:
[ 本帖最后由 s_mss 于 2006-6-22 11:28 编辑 ] 这个例子感觉上似是而非
给定tref 600度C 是计算热应力的参考温度
整个模型温度为20度C
计算出的应该是相较于600度C的热应力
可以认定为冷却到20度C的应力值吗?
不是很瞭解
最近有做一些残余应力的计算
希望有网兄能讨论一下 因为是在600时涂TiC,这时涂层内应该是无应力的,所以我认为计算出来的就是从600降到20度后的热应力。 无应力?
材料有加热不是就会膨胀
会有热应力?
还是说均匀温度分布所以没有热应力?
楼主可以提供参考的例子吗?
如果一开始是非均匀温度场呢?